Material Guide

Incoloy 825 vs Inconel 625: Differences, Properties and Uses

Metinox Overseas Team November 25, 2026 Incoloy 825 vs Inconel 625
Incoloy 825 vs Inconel 625

Incoloy 825 vs Inconel 625 is a question we get almost every week. Most buyers want to know if the cheaper alloy will do the job. Sometimes it will but often it won't.

Inconel 625 is stronger. It contains a minimum of 58% nickel and around 9% molybdenum. It has a PREN value of around 51. It is suitable for seawater and chloride environments. It can also be used at temperatures of up to around 980 oC.

Incoloy 825 contains less nickel (between 38 and 46%) and also has a minimum of 22% iron. It also contains a small quantity of copper. It has a PREN value of around 31 and so is not as suitable as Inconel 625 for chloride environments. However, it is extremely suitable for sulphuric and phosphoric acids. It is more economical and can be used up to around 540 oC.

Our simple rule is this: use Inconel 625 for chloride, high strength and/or high temperature applications. Use Incoloy 825 for acid environments where economy is an issue. Below we describe the differences in make-up, strength, corrosion, temperature, welding, standards and cost between Inconel 625 and Incoloy 825. This information is drawn from our extensive experience of supplying these materials as pipe & tube, nickel alloy flanges and fittings.

Incoloy 825 vs Inconel 625: Quick Comparison Table

Choose Inconel 625 when the job involves chlorides, seawater, high strength or temperatures above 540 °C. Choose Incoloy 825 when the job is mainly acid, the temperature is moderate and the budget matters.

Factor

Inconel Alloy 625

Incoloy Alloy 825

UNS number

N06625

N08825

Alloy family

Nickel, chromium, molybdenum, niobium

Nickel, iron, chromium, copper, molybdenum

Nickel content

58% minimum

38 to 46%

Strength

High

Moderate

Seawater and chloride pitting

Excellent

Fair

Sulphuric and phosphoric acid

Very good

Excellent

Typical upper service limit

About 980 °C (oxidation)

About 540 °C (pressure service)

Relative cost

Higher

Lower

Why "Inconel" and "Incoloy"?

Both are Special Metals trade names. Inconel alloys are nickel-chromium based with little iron, built for heat and severe corrosion. Incoloy alloys are nickel-iron-chromium based, using iron to cut cost while keeping good corrosion resistance. That family difference explains most of what follows.

What Is Inconel Alloy 625?

Inconel 625 (also called Alloy 625, UNS N06625) is a nickel-chromium-molybdenum alloy with added niobium. The molybdenum and niobium stiffen the metal's atomic structure, so it gains strength without any age-hardening heat treatment. That is why it holds up from cryogenic temperatures to very hot service, and why it resists fatigue so well.

Engineers reach for it when seawater, chloride-rich process streams or sour wells would destroy a lesser material. You will find it in subsea risers, flare tips, heat exchangers, aircraft ducting and chemical reactors. We supply Inconel 625 pipes and tubes in seamless and welded forms.

What Is Incoloy Alloy 825?

Incoloy 825 (Alloy 825, UNS N08825) is a nickel-iron-chromium alloy with added molybdenum, copper and titanium. Copper gives it a real advantage in sulphuric acid. Titanium ties up carbon, so the alloy resists intergranular attack after welding. Its high iron content also keeps it far cheaper than a high-nickel grade.

Alloy 825 is a workhorse in acid plants, pickling lines, pollution control scrubbers and oil and gas surface equipment. It is not built for the extreme strength or heat that 625 delivers, and that is the main trade-off. Our range includes Incoloy 825 pipes and tubes for process and heat exchanger duty.

Inconel 625 vs Incoloy 825 Chemical Composition

The Incoloy 825 vs Inconel 625 composition gap is clear: Alloy 625 has much more nickel and molybdenum, plus niobium.

Element (weight %)

Inconel 625

Incoloy 825

Nickel (Ni)

58.0 min

38.0 to 46.0

Chromium (Cr)

20.0 to 23.0

19.5 to 23.5

Iron (Fe)

5.0 max

22.0 min

Molybdenum (Mo)

8.0 to 10.0

2.5 to 3.5

Niobium (Nb) + Ta

3.15 to 4.15

—

Copper (Cu)

—

1.5 to 3.0

Titanium (Ti)

0.40 max

0.60 to 1.20

Carbon (C)

0.10 max

0.05 max

Manganese (Mn)

0.50 max

1.00 max

Silicon (Si)

0.50 max

0.50 max

Aluminium (Al)

0.40 max

0.20 max

Cobalt (Co)

1.0 max

—

Sulphur (S)

0.015 max

0.030 max

Three points matter most in practice:

  • Molybdenum: about 9% in 625 against about 3% in 825. This is the main reason 625 resists pitting and crevice corrosion so much better.
  • Niobium: only 625 has it. It adds strength and stabilises the weld zone.
  • Copper and iron: only 825 has meaningful amounts. They help in sulphuric acid and bring the price down.

Mechanical Properties: Strength of Alloy 625 vs Alloy 825

Inconel 625 is clearly the stronger alloy.

Property

Inconel 625

Incoloy 825

Tensile strength, min

827 MPa (120 ksi)

586 MPa (85 ksi)

Yield strength 0.2%, min

414 MPa (60 ksi)

241 MPa (35 ksi)

Elongation, min

30%

30%

Tensile strength, typical annealed

About 930 MPa

About 690 MPa

Yield strength 0.2%, typical annealed

About 517 MPa

About 310 MPa

In plain terms, 625 has roughly 40% higher tensile strength and about 70% higher yield strength.

Physical Properties of Alloy 625 vs Alloy 825

Property

Inconel 625

Incoloy 825

Density

8.44 g/cm³

8.14 g/cm³

Melting range

1290 to 1350 °C

1370 to 1400 °C

Thermal conductivity, room temperature

9.8 W/m·K

11.1 W/m·K

Mean thermal expansion, 20 to 100 °C

12.8 µm/m·°C

14.0 µm/m·°C

Elastic modulus

About 205 GPa

About 196 GPa

Alloy 825 melts at a slightly higher temperature, but that does not make it the better alloy for hot service. Strength and creep resistance at temperature decide that, and 625 wins on both. The higher thermal conductivity of 825 is a small plus in heat exchangers. For help with wall thickness and weight, see our pipe size chart.

Corrosion Resistance: Inconel 625 vs Incoloy 825

A quick way to rank pitting resistance is PREN (pitting resistance equivalent number):

PREN = %Cr + 3.3 × %Mo + 16 × %N

Environment

Inconel 625

Incoloy 825

Seawater, pitting and crevice corrosion

Excellent

Fair

Chloride stress corrosion cracking

Excellent

Very good

Sulphuric acid

Very good

Excellent

Phosphoric acid

Very good

Excellent

Nitric acid

Excellent

Very good

Hydrochloric acid

Limited

Limited

Sour gas (H₂S), NACE MR0175 / ISO 15156

Suitable grades available

Suitable grades available

Oxidising atmospheres at high temperature

Excellent

Good

Seawater and chlorides favour 625 by a wide margin. Sulphuric and phosphoric acid favour 825, where the copper content does real work. Neither alloy is a first choice for hydrochloric acid, where a Hastelloy grade is usually safer. Our guide on Inconel vs Hastelloy nickel alloy pipes explains when to step up.

Temperature Performance of Inconel 625 and Incoloy 825

Inconel 625 keeps its strength and resists oxidation up to about 980 °C, and it stays tough down to cryogenic temperatures. For pressure-containing parts, design codes limit allowable stress at the upper end, so most engineered 625 lines run well below its oxidation ceiling.

Incoloy 825 is usually rated to about 540 °C (1000 °F) for pressure service. Above that, its lower strength and creep resistance make it a poor fit, and 625 or an alloy such as Incoloy 800H is the better route. Always check the allowable stress tables in your design code before you fix the wall thickness.

Both alloys keep their toughness at very low temperatures because they are austenitic, so neither suffers the ductile-to-brittle transition seen in carbon steel.

Weldability and Fabrication of Alloy 625 vs Alloy 825

Both alloys weld well by gas tungsten arc, shielded metal arc and gas metal arc methods, and neither normally needs post-weld heat treatment in standard service. The differences are small but worth knowing.

Filler metal:

Alloy 625 is welded with ERNiCrMo-3 (AWS A5.14). Alloy 825 is commonly welded with ERNiFeCr-1, and ERNiCrMo-3 is often chosen when the weld needs extra pitting resistance. ERNiCrMo-3 is also the usual choice when joining 625 to 825.

Heat control:

Use low heat input and keep the interpass temperature at or below about 150 °C. Molten nickel alloys flow sluggishly, so bead placement matters.

Cleanliness:

Remove oil, paint, marking ink and anything containing sulphur before welding. Sulphur causes cracking in nickel alloys.

Back purging:

Purge the root side with argon on both alloys to protect the inside of the weld.

Forming and machining:

Alloy 625 work-hardens quickly and needs rigid setups and sharp tools. Alloy 825 forms and machines more easily.

Heat treatment:

Alloy 625 is supplied annealed (Grade 1, typically above 870 °C) or solution annealed (Grade 2, typically above 1090 °C) for high-temperature creep service. Alloy 825 is supplied in the stabilised-annealed condition at about 940 °C, which keeps carbon tied up with titanium. Neither alloy is normally post-weld heat treated in corrosion service

UNS N06625 vs UNS N08825: Standards and Equivalents

Buying to the right specification matters as much as choosing the right alloy. These are the standards most often called out on purchase orders.

Product form

Inconel 625 (UNS N06625)

Incoloy 825 (UNS N08825)

Seamless pipe and tube

ASTM B444 / ASME SB444

ASTM B423 / ASME SB423

Welded pipe

ASTM B705

ASTM B705

Welded tube

ASTM B704

ASTM B704

Plate, sheet and strip

ASTM B443

ASTM B424

Bar and rod

ASTM B446

ASTM B425

Buttweld fittings

ASTM B366 WPNCMC

ASTM B366 WPNICMC

Forged flanges and fittings

ASTM B564

ASTM B564

Werkstoff number

2.4856

2.4858

EN designation

NiCr22Mo9Nb

NiCr21Mo

For connecting hardware, see our Alloy 625 flanges, Alloy 825 flanges and Inconel pipe fittings.

Incoloy 825 vs Inconel 625 Price: What Drives the Difference

Alloy 825 is normally the cheaper of the two. It uses less nickel and molybdenum and contains no niobium, so its raw material cost is lower. Alloy 625 carries a premium because those three elements are expensive and their prices move with the metals market.

Price per kilogram is only part of the story. A thinner 625 wall can cut weight, and a longer service life can cut replacement costs. On the other hand, paying for 625 in a mild acid line is money wasted. If the process is purely acidic and chloride is low, Alloy 825 or SS 904L pipes may do the job for less. Because nickel and molybdenum prices change weekly, current figures are best checked with your supplier.

Applications of Incoloy 825 vs Inconel 625 by Industry

Industry

Inconel 625

Incoloy 825

Oil and gas pipes and tubes

Subsea risers, flowlines, high-pressure sour wells

Surface piping, heat exchangers, gas processing

Chemical processing pipes

Reactors and lines handling chlorides and mixed acids

Sulphuric and phosphoric acid lines, pickling tanks, coolers

Marine and offshore pipes

Seawater systems, heat exchangers, fasteners

Limited use, mostly freshwater and acid-side services

Power generation

Flue gas desulphurisation, boiler components

Scrubbers and cooling water systems

Aerospace

Exhaust ducting, thrust reverser parts

Rarely used

Pollution control

Aggressive stack liners

Acid gas scrubbers, waste treatment

Common Specification Mistakes We See

After years of reviewing enquiries for these two alloys, the same errors come up again and again:

  • Over-specifying 625 for acid service: A sulphuric acid line at moderate temperature with little chloride rarely needs 625. Alloy 825 does the job, and the saving on a large project can be substantial.
  • Using 825 in warm, stagnant seawater: It looks fine at first, but crevice corrosion often shows up at flange faces and under gaskets within a few years.
  • Mixing up fitting grades: Alloy 625 fittings are ASTM B366 WPNCMC and Alloy 825 fittings are WPNICMC. A wrong grade on the purchase order leads to rejected mill certificates and delays.
  • Not stating the 625 grade: Leaving out B444 Grade 1 or Grade 2 can bring in material with very different strength minimums from what the designer assumed.

How to Choose Between Inconel 625 and Incoloy 825

Choose Inconel Alloy 625 when:

  • The fluid contains chlorides, seawater or brine.
  • You need high strength, fatigue resistance or thin walls.
  • Service temperature goes above about 540 °C.
  • The line is critical and a failure would be costly.

Choose Incoloy Alloy 825 when:

  • The main hazard is sulphuric, phosphoric or other reducing acids.
  • Temperature stays moderate and pressure is not extreme.
  • Chloride levels are low and the budget is tight.
  • You want easy fabrication and good resistance to stress corrosion cracking.

If your process has…

Start with

Seawater or high chloride

Inconel 625

Sulphuric or phosphoric acid, low chloride

Incoloy 825

High temperature and high pressure

Inconel 625

Moderate temperature, cost-sensitive

Incoloy 825

Hydrochloric acid or mixed severe acids

A Hastelloy grade, see Hastelloy pipes and tubes

Seawater with a tighter budget

Consider super duplex steel pipes

Still unsure? Share your fluid, temperature and pressure with our materials team for a free second opinion on grade selection.

Ask our materials team

Explore Alloy 625 and Alloy 825 Products

Metinox Overseas supplies both alloys in the forms most plants buy: seamless and welded pipes and tubes, forged flanges and fittings. Browse our Inconel flanges, explore our nickel alloy pipe fittings, or see the wider special alloys pipes and tubes range. Material is supplied with mill test certificates.

If you are drafting a specification, list the grade, size, wall thickness or schedule and the ASTM standard together; it prevents most of the mix-ups described above.

FAQs on Incoloy 825 vs Inconel 625

Not in every case. Inconel 625 is stronger and handles seawater, chlorides and high temperature better. Incoloy 825 is better value in sulphuric and phosphoric acid. The right answer depends on your process.

Composition. Inconel 625 has at least 58% nickel, about 9% molybdenum and added niobium. Incoloy 825 has 38 to 46% nickel, at least 22% iron and added copper. That chemistry drives strength, corrosion behaviour and price.

Inconel 625. Its PREN is about 51 against about 31 for Incoloy 825, so it resists pitting and crevice corrosion far better in seawater and chloride-bearing fluids.

Incoloy 825 is usually cheaper because it contains less nickel and molybdenum and no niobium. Nickel and molybdenum prices change, so check current figures with your supplier.

Sometimes. It can work in moderate-temperature acid service with low chloride. It should not replace 625 in seawater, high-strength or high-temperature duty, because its pitting resistance and strength are lower.

Yes. Both have grades listed in NACE MR0175 / ISO 15156 for hydrogen sulphide environments. Alloy 625 is preferred where higher strength or temperature is needed. Always confirm the condition and limits for your exact service.

Yes. The joint is routine, and ERNiCrMo-3 filler is the usual choice because it matches or exceeds the corrosion resistance of both base metals.

For pressure-containing parts, Incoloy 825 is generally limited to about 540 °C (1000 °F). Above that, Inconel 625 or Incoloy 800H is the better choice.

Conclusion: Inconel Alloy 625 or Incoloy Alloy 825?

Inconel 625 is the premium choice for chlorides, strength and heat, while Incoloy 825 is the sensible choice for acid duty at moderate temperatures. Match the alloy to the environment first and the budget second, and you will avoid both overspending and early failure.

Next, see how these alloys compare with Hastelloy in our Inconel vs Hastelloy guide, or browse more material comparisons on the Metinox blog.

Inconel and Incoloy are trademarks of Special Metals Corporation. They are used here for reference only; the generic names Alloy 625 and Alloy 825 apply equally.

Looking to Enquire or Place an Order?

Share your requirement and our team will respond with pricing, availability, and technical details.

Incoloy 825 vs Inconel 625